Сохранить в закладки:
C | Mn | Si | P | S | Cu | Ni | Co | V | Fe | ||||||
(≤) | |||||||||||||||
0.04 | 0.3 | 0.3 | 0.02 | 0.02 | 0.2 | 0.5 | 49.0-51.0 | 0.80-1.80 | Bal. |
Density (g/cm3) | Resistivity (ΜΩ•m) | Curie point (℃) | remanence (T) | Yield Strength (MPa) | Tensile strength (Mpa) | Elongation (%) | Elastic Modulus Ksi | Magnetostriction coefficient |
8.2 | 0.4 | 980 | 1.45 | 1280 | 1340 | 1 | 3x103 | 60x10-6 |
Product form | Magnetic induction intensity at different magnetic field strength (A/m)/T | Coercivity Hc/(A/m) | ||||||||||
B400 | B800 | B1600 | B2400 | B4000 | B8000 | |||||||
≥ | ≤ | |||||||||||
Cold rolled strip | 1.6 | 1.8 | 2 | 2.1 | 2.15 | 2.2 | 128 | |||||
Wire, forged (rolled) material | ... | ... | ... | 2.05 | 2.15 | 2.2 | 144 |
Temperature | Coefficient of expansion | ||||
68°F | 20°C | -6/°F | 10-6/℃ | ||
392 | 200 | 5.28 | 9.5 | ||
752 | 400 | 5.61 | 10.1 | ||
1112 | 600 | 5.83 | 10.5 | ||
1472 | 800 | 6.28 | 11.3 |
Form | Specification/mm | Delivery status |
Bar | 8.0-30.0 | Hot rolled |
30.0-180.0 | Hot forging | |
Plate | 3.5-30.0 | Hot rolled |
30.0-40.0 | Hot forging | |
Strip | 0.05-1.0 | Cold rolled |